How to weld > Preheating and interpass temperature

Attaining and measuring the preheating temperature and recommended preheating operation

The required preheating temperature can be achieved through various methods. Electric preheater elements positioned around the prepared joint are often preferred, as they allow for uniform heating of the area, see illustration below. Temperature monitoring can be done using a contact thermometer, ensuring accuracy during the heating process. Note the following procedures:
  • A minimum waiting time of 2 minutes per 25 mm (2 minutes per 1 inch) thickness should be observed before measuring the preheating temperature. 
  • The minimum preheating temperature should be obtained in an area of 75 + 75 mm (3” + 3”) around the intended weld joint. 
  • Measure the interpass temperature on the weld metal at the intended start position of the weld pass or immediately adjacent to the parent metal.

Recommended preheating operation.

Contact Technical support


The information in this report is only applicable to SSAB’s products and should not be applied to any other products than original SSAB products. 


This report provides general results and recommendations for SSAB steel products. This report is subject to SSAB’s Terms of Use. It shall be the user's responsibility to verify that the information contained herein is correct and is suitable to be used for the particular purpose and application of the user. The report is intended to be used by professional users only who possess adequate expertise, qualification and knowledge for the safe and correct use of the results and recommendations in this report. This report is provided “as is”. The use of the report is at user’s own discretion and risk and that users will be solely responsible for any use of this report. SSAB disclaims any liability for the content or potential errors of this report, including but not limited to warranties and condition of merchantability or fitness for a particular purpose or suitability for individual applications. SSAB shall not be liable for any kind of direct or indirect damages and/or costs related to or arising therefrom, whether special, incidental, consequential or directly or indirectly related to the use of, or the inability to use, the report or the content, information or results included therein. 