How to weld > Preheating and interpass temperature

Factors Affecting Preheat and Interpass Temperatures

When plates, sheets, round bars and tubes of different thicknesses but of the same steel grade are welded together, the thicker plate determines the required preheating and interpass temperatures; see illustration below.

Recommended location of the root pass in relation to the centerline of the cross section. X should be 5 mm smaller than Y/2.

When different steel types are welded together, the plates, sheets, round bars and tubes requiring the highest preheating temperature determines the required preheat and interpass temperatures.

The tables below are applicable for heat inputs of 1.7 kJ/mm (43.2 kJ/inch) or higher. If heat inputs of 1.0–1.69 kJ/mm (25.4–42.9 kJ/inch) are used, we recommend an increase of the temperature by 25°C (77°F) above the recommended preheating temperature. Furthermore, these preheating recommendations is valid for consumables recommended by SSAB with a max diffusible hydrogen content of 5 ml/100 g weld metal.

If a lower heat input than 1.0 kJ/mm (25.4 kJ/inch) is applied, we recommend that you use SSAB’s WeldCalc to calculate the recommended minimum preheating temperature.

If the ambient humidity is high or the temperature is below 5°C (41°F), the lowest recommended preheating temperatures given in the tables below should be increased by 25°C (77°F).

For plates thicker than 25 mm (0.984”), and joint geometries, where the root pass is close to the centerline of the plate such as double-V butt welds, we recommend locating the root pass approximately 5 mm (0.197”) away from the centerline of the plate, see illustrated above.

Contact Technical support


The information in this report is only applicable to SSAB’s products and should not be applied to any other products than original SSAB products. 


This report provides general results and recommendations for SSAB steel products. This report is subject to SSAB’s Terms of Use. It shall be the user's responsibility to verify that the information contained herein is correct and is suitable to be used for the particular purpose and application of the user. The report is intended to be used by professional users only who possess adequate expertise, qualification and knowledge for the safe and correct use of the results and recommendations in this report. This report is provided “as is”. The use of the report is at user’s own discretion and risk and that users will be solely responsible for any use of this report. SSAB disclaims any liability for the content or potential errors of this report, including but not limited to warranties and condition of merchantability or fitness for a particular purpose or suitability for individual applications. SSAB shall not be liable for any kind of direct or indirect damages and/or costs related to or arising therefrom, whether special, incidental, consequential or directly or indirectly related to the use of, or the inability to use, the report or the content, information or results included therein. 

Copyright 2026