How to weld > Shielding gas

MAG and TIG Welding of Hardox® and Strenx®

The shielding gases proposed in the table below for MAG and TIG welding of Hardox® and Strenx® are well balanced in order to support a high-quality welding performance.

If Hardox® and Strenx® grades are welded to other types of steel the same gas types may be applied.

Welding method
Welding method
 MAG, solid wire
Arc type
 Short arc
Position
 All positions
Shielding gas [weight %]
 18-25% CO2, rest Ar
Welding method
Welding method
 MAG, cored wire
Arc type
 Short arc
Position
 All positions
Shielding gas [weight %]
 18-25% CO2, rest Ar
Welding method
Welding method
 MAG, solid wire
Arc type
 Spray arc
Position
 Horizontal (PA, PB, PC)
Shielding gas [weight %]
 15-20% CO2, rest Ar
Welding method
Welding method
 MAG, MCAW
Arc type
 Spray arc
Position
 All positions
Shielding gas [weight %]
 15-20% CO2, rest Ar
Welding method
Welding method
 MAG, MCAW
Arc type
 Spray arc
Position
 Horizontal (PA, PB, PC)
Shielding gas [weight %]
 15-20% CO2, rest Ar
Welding method
Welding method
 Robotic and automatic MAG
Arc type
 Spray arc
Position
 Horizontal (PA, PB, PC)
Shielding gas [weight %]
  8-18% CO2, rest Ar
Welding method
Welding method
 TIG
Arc type
 Spray arc
Position
 All positions
Shielding gas [weight %]
 100% Ar

Suggestions of different gas mixtures for welding the Hardox® and Strenx® grades.

Note that shielding gases other can also be used. The consumable manufacturer can also specify a certain shielding gas composition for a specific consumable. In such a case, the recommendations for the consumable should be applied.

Gas flow

Gas flow can be optimized in order to get a well-balanced welding performance. Too little gas flow results in inadequate protection of the melt. Excessive gas flow can become turbulent thus deteriorating the gas protection.

The gas flow for all welding methods based on shielding gases, as a rule of thumb, can be set by using the same number of the gas flow measured in l/min as the inner diameter of the nozzle measured in mm.

Category and tags

How to weldShielding gas

Contact Technical support


The information in this report is only applicable to SSAB’s products and should not be applied to any other products than original SSAB products. 


This report provides general results and recommendations for SSAB steel products. This report is subject to SSAB’s Terms of Use. It shall be the user's responsibility to verify that the information contained herein is correct and is suitable to be used for the particular purpose and application of the user. The report is intended to be used by professional users only who possess adequate expertise, qualification and knowledge for the safe and correct use of the results and recommendations in this report. This report is provided “as is”. The use of the report is at user’s own discretion and risk and that users will be solely responsible for any use of this report. SSAB disclaims any liability for the content or potential errors of this report, including but not limited to warranties and condition of merchantability or fitness for a particular purpose or suitability for individual applications. SSAB shall not be liable for any kind of direct or indirect damages and/or costs related to or arising therefrom, whether special, incidental, consequential or directly or indirectly related to the use of, or the inability to use, the report or the content, information or results included therein. 

Copyright 2026